Hastelloy Alloy is a kind of nickel based high temperature alloy.
Yesom Group offers Hastelloy Alloy in shape of wire, bar, plate, strip, coil, flange, etc.
	Alloy Grade: Hastelloy C-4 ,  Hastelloy C-22 ,  Hastelloy C-276 , Hastelloy C-2000 , 
                      Hastelloy B , Hastelloy B-2 , Hastelloy B-3 , Hastelloy X
 
	
 
Hastelloy C-276
	
	
		
			
				 
			
					 Hastelloy C-276 (UNS 10276 / W.Nr.2.4819 / NS336)
				 
			
				 
			
					 Chemical Composition %
				 
				
					 Ni: Margin
				 
				
					 Cr: 14.5-16.5
				 
				
					 Fe: 4-7
				 
			
				 
			
					 W: 3-4.55
				 
				
					 Mo: 15-17
				 
				
					 Mn: ≤1
				 
			
				 
			
					 Co: ≤2.5
				 
				
					 C: ≤0.01
				 
				
					 Si: ≤0.08
				 
			
				 
			
					 P: ≤0.04
				 
				
					 S: ≤0.03
				 
				
					 V: ≤0.35
				 
			
				 
			
					 Melting Point ℃
				 
				
					 1325-1370
				 
			
				 
			
					 Density g/cm3
				 
				
					 8.9
				 
			
				 
			
					 Executive Standards
				 
				
					 ASTM: B575
				 
			
				 
		
	
					 Application Area
				 
				
					 Bleaching containers, equipment and components operating in acidic gas environments, reactors for acetic acid and acidic products, and sulfuric acid condensers in the pulp and paper industry
				 
			
	
Designations: AWS 054
	
Specifications: ASTM B574 , ASTM B575 , ASTM B619
	
Alloy Details
		
		 
				 
			 
				Heat treatment of finished parts
			 
				 
			 
				Properties
			 
				 
			 
			The above information is typical. If you require different please ask.
		
					
						
			
							 
						
								Density
							 
							
								Melting Point
							 
							
								Coefficient of Expansion
							 
							
								Modulus of Rigidity
							 
							
								Modulus of Elasticity
							 
						
							 
						
								8.89 g/cm³
							 
							
								1370 °C
							 
							
								11.2 μm/m °C (20 – 100 °C)
							 
							
								78.6 kN/mm²
							 
							
								205.5 kN/mm²
							 
						
							 
					
				
								0.321 lb/in³
							 
							
								2500 °F
							 
							
								6.2 x 10-6 in/in °F (70 – 212 °F)
							 
							
								11400 ksi
							 
							
								29806 ksi
							 
						
					
						
			
							 
						
								Condition as supplied by AWI
							 
							
								Type
							 
							
								Temperature
							 
							
								Time
							 
							
								Cooling
							 
						
							 
					
				
								Annealed or Spring Temper
							 
							
								Stress Relieve
							 
							
								400 – 450 °C (750 – 840 °F)
							 
							
								2 Hr
							 
							
								Air
							 
						
					
						
			
							 
						
								Annealed
							 
							
								 
							 
							
								 
							 
						
							 
						
								Approx. tensile strength
							 
							
								<1050 N/mm²
							 
							
								<152 ksi
							 
						
							 
					
				
								Approx. operating temperature depending on loading and environment
							 
							
								-200 to +400 °C
							 
							
								-330 to +750 °F
							 
						
					
						
			
							 
						
								Spring Temper
							 
							
								 
							 
							
								 
							 
						
							 
						
								Approx. tensile strength
							 
							
								1300 – 1700 N/mm²
							 
							
								189 – 247 ksi
							 
						
							 
					
				
								Approx. operating temperature depending on loading and environment
							 
							
								-200 to +400 °C
							 
							
								-330 to +750 °F
							 
						
	
	 
 
  
	